English
Welcome to opelink.com

Single-Component Thermal Gel -18 W/m·K for Optical Modules

Item No.: Y-TIM-002
Single-component heat-cure thermal gel: 18 W/m·K, ~200 µm bond line, ~70 psi stress, low outgassing for optical modules and sensitive packages.
Description Parameters

Product Overview

This product is a single-component, heat-cure thermal gel developed for thermal interfaces in optical modules and other densely packed electronic assemblies. The material is supplied as a dispensable paste and remains in place after dispensing without slumping, so that a defined, thin bond line can be formed before cure. A short heat-cure step converts the paste into a soft, highly compliant gel that accommodates thermal expansion mismatch and mechanical tolerance stack-up.
The formulation combines a thermal conductivity of 18 W/m·K with a minimum achievable bond line thickness (BLT) of approximately 200 μm. Its very low compression stress — about 70 psi at 0.2 mm — keeps the load on the die, the optical sub-assembly and the package within safe limits, while the residual stress after compression settles at about 8.1 psi. Low oil bleed, low outgassing and stable thermal resistance under long-term aging make the product suitable for applications in which optical surfaces and long service life are critical.

Single-Component Thermal Gel -18 W/m·K for Optical Modules
Key Features

  1. High thermal conductivity of 18 W/m·K (ASTM D5470, 80 °C / 40 psi) with a bond line of about 200 μm.
  2. Thin, uniform bond line down to approximately 200 μm, with a measured maximum of 0.188–0.195 mm across batches.
  3. Ultra-low compression stress — about 70 psi at 0.2 mm compression and about 8.1 psi residual stress — minimising mechanical load on fragile components.
  4. Low oil bleed of 1.0–1.5 mm on grid paper after cure, which limits contamination of optical and electrical surfaces.
  5. Low outgassing — TML 0.05 % and CVCM 0.01 % (ASTM E595); no condensable volatiles were observed during cure at 100 °C.
  6. Non-slumping, shape-stable deposit — the paste stays where it is dispensed and does not flow into adjacent areas before cure.
  7. Suitable for automated dispensing at 20–30 g/min through a 30 cc syringe at 90 psi, with consistent batch-to-batch output.
  8. Proven long-term reliability — thermal resistance changes by 3 % or less after 2000 h at 100 °C, 2000 h at 85 °C / 85 % RH and 2000 thermal cycles between −40 °C and 125 °C.
  9. Long room-temperature working life — the uncured gel remains workable at room temperature for up to 96 h, which supports multi-station line architectures.

Typical Applications

The product was characterised against the thermal requirements of optical modules, and the following uses follow directly from that characterisation work:
  1. Optical transceiver and photonic modules — thermal interface between the optical sub-assembly and the module housing, where a bond line of about 0.3 mm is typically used and thermal margin is retained.
  2. Stress-sensitive optical and electronic assemblies — the low compression and residual stress make the gel suitable for packages that cannot tolerate high clamping forces.
  3. Automated dispensing and high-volume assembly lines — stable extrusion rate and non-slumping behaviour support screen-free, needle-based dispensing.
  4. Assemblies with exposed optical or electrical surfaces — low oil bleed and low outgassing reduce the risk of fogging or contamination of optical surfaces.
Applications outside the scope described above should be qualified by the user against the specific package, dispense geometry and cure profile. Please contact the supplier for application-specific evaluation.

FAQ

What is a single-component heat-cure thermal gel?

A single-component heat-cure thermal gel is a dispensable paste that stays in place after dispensing and becomes a soft, compliant gel when heated.
  1. No mixing and no pot-life control are required before dispensing.
  2. The paste does not slump, so a defined bond line forms before cure.
  3. Cure converts the paste into a low-stress gel that absorbs tolerance stack-up.
  4. The material is supplied frozen and thawed before use.

Which bond line thickness suits optical module assemblies?

Optical module designs typically use a 0.3 mm bond line, where measured thermal resistance is 0.200 °C/W.
  1. 0.2 mm gives 0.144 °C/W, the thinnest characterised point.
  2. 0.3 mm gives 0.200 °C/W and retains design margin.
  3. 0.5 mm gives 0.311 °C/W; 1.0 mm gives 0.589 °C/W.
  4. Values are ASTM D5470 at 80 °C and 40 psi.

Does the gel meet ASTM E595 outgassing limits?

TML is 0.05 %, RML 0.04 %, CVCM 0.01 % and WVR 0.00 %, all measured at 125 °C for 24 h.
  1. No condensable volatiles were detected from 10 to 60 min of cure at 100 °C.
  2. Low outgassing limits fogging of nearby optical surfaces.
  3. Test reports are available on request.

Can RoHS and REACH declarations be provided?

RoHS and REACH declarations are not stated in this datasheet and must be requested with the quotation.
  1. The certificate of analysis is issued with each batch.
  2. The disclaimer places regulatory compliance on the user.
  3. Confirm the document revision against the label before design release.

How are voids avoided during dispensing?

Voids are avoided by keeping the working gap at or above the bond line and dispensing with a correctly sized needle.
  1. The working gap shall not be smaller than the bond line thickness.
  2. Check that the needle is not blocked or partly cured before a run.
  3. Thaw the cartridge completely at 25 ± 2 °C for at least 1 h.
  4. Dispense in a clean, draught-free area free of dust and lint.

How should frozen cartridges be stored and thawed?

Store at −40 °C to −18 °C in the sealed container and thaw at 25 ± 2 °C for at least 1 h.
  1. Total thaw cycles shall not exceed two.
  2. Do not open the cartridge or accelerate thawing with heat, hot water or a microwave.
  3. Keep the container closed and upright to prevent moisture pick-up.
  4. Shelf life is stated on the label and certificate of analysis.

How long does thermal resistance stay stable under stress?

Thermal resistance changed by 3 % or less after 2000 h at 100 °C, 2000 h at 85 °C / 85 % RH and 2000 thermal cycles.
  1. Cycling ran between −40 °C and 125 °C, 1 h per cycle.
  2. No delamination, cracking or pumping-out was observed.
  3. A change of 3 % or less is treated as stable.
  4. Bonded specimens also passed 1000 h and 1000 cycles.

What information is needed for a quotation?

A quotation is prepared from the package, working gap, target bond line, cure schedule and required documents.
  1. State the working gap and the target bond line thickness.
  2. State the cure schedule: 85 °C for 3 h or 100 °C for 1 h.
  3. List required documents such as the certificate of analysis or test reports.
  4. Delivery timing is confirmed by the supplier once these details are received.

1.Typical Properties

The values below are typical values obtained from production batches under the stated test conditions. They are provided for reference and engineering evaluation and are not specification limits.
Table 1. Typical properties of the thermal gel
Property Unit Typical Value Test Method Test Condition
Thermal conductivity W/m·K 18 ASTM D5470 (LW-9389) 80 °C, 40 psi
Bond line thickness (BLT) μm ≈ 200 ASTM D5470 (LW-9389) 30 °C, 20 psi zeroing; constant pressure
Density g/cm³ 3.20 GB/T 533-2008 Specific gravity before cure; immersion after cure
Extrusion rate g/min 20–30 Supplier in-house method 30 cc syringe, 90 psi, 1 min
Dielectric strength kV/mm 3.6 ASTM D149-20 50 Hz AC
Compression stress psi ≈ 70 Supplier in-house method 10 mm/min, 1.0 mm → 0.2 mm
Residual stress psi ≈ 8.1 Supplier in-house method 3 min after compression to 0.2 mm
Adhesive strength psi ≈ 30 GB/T 528-2009 Cross tensile (pull-off), 10 mm/min; cohesive failure
Coefficient of thermal expansion μm/m·°C 79.04 GB/T 36800.2-2018 TMA, 25–100 °C, 10 °C/min
Hardness Shore OO 59–61 Supplier in-house method Cured specimen, 25 °C
Total mass loss (TML) % 0.05 ASTM E595 125 °C, 24 h
Recovered mass loss (RML) % 0.04 ASTM E595 125 °C, 24 h
Collected volatile condensable materials (CVCM) % 0.01 ASTM E595 125 °C, 24 h
Water vapour regained (WVR) % 0.00 ASTM E595 125 °C, 24 h; pre-conditioned 23 °C / 50 % RH
Note: All values are typical data from production batches and are not guaranteed specification limits. Values marked with the supplier in-house method are documented in the corresponding test report, available on request. BLT is the minimum thickness reached by an unconstrained sample under constant pressure at 30 °C after zeroing at 20 psi; the maximum measured value was 0.188–0.195 mm over three batches. Density: 3.201 g/cm³ before cure (specific-gravity method), 3.198 g/cm³ after 85 °C cure and 3.196 g/cm³ after 100 °C cure (immersion), equivalent to a volume shrinkage of 0.094 % and 0.156 %; both methods carry a measurement uncertainty and the figures are for reference. Compression stress was measured on a 25.3 × 25.3 mm contact area; the residual stress peak value was 9.39 psi. Adhesive strength was measured on 25.4 × 25.4 × 0.35 mm nickel-plated specimens cured at 100 °C for 1 h or 85 °C for 3 h, and all joints failed cohesively in the gel. CTE was determined over 25–100 °C only at a heating rate of 10 °C/min under 0.05 N. Outgassing data (TML, RML, CVCM) were obtained at 125 °C for 24 h under approximately 10⁻⁶ Torr; WVR was measured after 24 h at 50 % relative humidity.

2.Thermal Resistance versus Bond Line Thickness

Thermal resistance was measured on a steady-state thermal resistance tester (ASTM D5470) with the hot side at 80 °C and a contact pressure of 40 psi. Three samples were tested at each thickness and the table reports the individual readings together with their average.
Table 2. Thermal resistance as a function of bond line thickness
Bond line thickness (mm) R₁ (°C/W) R₂ (°C/W) R₃ (°C/W) Average (°C/W)
0.2 0.142 0.146 0.144 0.144
0.3 0.198 0.203 0.199 0.200
0.5 0.309 0.314 0.310 0.311
0.7 0.420 0.425 0.421 0.422
1.0 0.587 0.592 0.588 0.589
1.5 0.864 0.870 0.866 0.867
Note: Measured per ASTM D5470 at 80 °C and 40 psi. The thermal conductivity of 18 W/m·K was obtained by linear regression of the 0.5 mm, 1.0 mm and 1.5 mm data points on the thickness–thermal resistance curve; the 0.2 mm, 0.3 mm and 0.7 mm points were not used in the fit. At the 0.3 mm bond line typical of optical module designs, the measured thermal resistance leaves design margin.

3.Reliability

Reliability was assessed by monitoring the change in thermal resistance before and after each stress. In all three test regimes the change remained at or below 3 %, and no delamination, cracking or pumping-out of the gel was observed.
Table 4. Reliability test summary
Test Condition Duration Acceptance criterion Result
High-temperature aging 100 °C 2000 h ΔRₜₕ ≤ 3 % Pass
Damp heat 85 °C / 85 % RH 2000 h ΔRₜₕ ≤ 3 % Pass
Thermal cycling −40 °C ↔ 125 °C
(15 min dwell, 15 min ramp, 1 h/cycle)
2000 cycles ΔRₜₕ ≤ 3 % Pass
Note: Thermal resistance was measured per ASTM D5470 at 80 °C and 40 psi before and after each stress. ΔRₜₕ is the relative change of thermal resistance; a change of 3 % or less is considered stable. Longer aging runs (1000 h and 1000 cycles) were also performed on bonded specimens and showed no separation of the bond line.

7.1  Volatile Condensable Materials

Cured samples were held at 100 °C and inspected at 10, 20, 30 and 60 min. No condensable volatiles were observed on the cooled collector at any of these intervals, which is consistent with the low TML (0.05 %) and CVCM (0.01 %) values reported in Table 1.

7.2  Oil Bleed and Migration

The extent of oil migration was measured on grid paper. A freshly dispensed deposit shows an oil mark of about 1.0 mm after 4 h at room temperature; after cure the mark measures 1.0–1.5 mm and stays within that range from day 1 to day 7. The bleed is therefore self-limiting and remains local to the deposit, which is important where the gel is dispensed close to optical surfaces or electrical contacts.

Review

Taily
Nov 13, 2026
We've received the samples and have asked our lab to run the validation.
 1